东北大学学报(自然科学版) ›› 2023, Vol. 44 ›› Issue (4): 517-523.DOI: 10.12068/j.issn.1005-3026.2023.04.008

• 材料与冶金 • 上一篇    下一篇

CaO-SiO2-Al2O3-Na2O-MgO系模铸保护渣微观结构解析

王震1,2, 姜茂发1,2, 刘承军1,2, 闵义1,2,3   

  1. (1. 多金属共生矿生态化冶金教育部重点实验室, 辽宁 沈阳110819;2. 东北大学 冶金学院, 辽宁 沈阳110819; 3. 海洋装备用金属材料及其应用国家重点实验室, 辽宁 鞍山114021)
  • 发布日期:2023-04-27
  • 通讯作者: 王震
  • 作者简介:王震(1998-),男,河北张家口人,东北大学硕士研究生; 姜茂发(1955-),男,山东栖霞人,东北大学教授,博士生导师; 刘承军(1974-),男,河南获嘉人,东北大学教授,博士生导师; 闵义(1972-),男,辽宁海城人,东北大学教授,博士生导师.
  • 基金资助:
    国家自然科学基金资助项目(51974075).

Microstructure Analysis of Mold Flux of Cao-SiO2-Al2O3-Na2O-MgO System for Ingot Casting

WANG Zhen1,2, JIANG Mao-fa1,2, LIU Cheng-jun1,2, MIN Yi1,2,3   

  1. 1. Key Laboratory for Ecological Metallurgy of Multimetallic Ministry
  • Published:2023-04-27
  • Contact: MIN Yi
  • About author:-
  • Supported by:
    -

摘要: 为明晰化学成分变化对模铸保护渣物性的影响机制,采用Raman光谱对CaO-SiO2-Al2O3-Na2O-MgO系熔融模铸保护渣的微观结构进行了解析.熔体结构解析结果表明,熔渣中存在Q0Si,Q1Si,Q2Si,Q3Si,Q4Si五种硅氧四面体结构和Q2Al,Q3Al,Q4Al三种铝氧四面体结构,随着碱度升高和Al2O3质量分数减小,高聚合度四面体结构向低聚合度转变,熔渣非桥氧数增多,聚合程度降低.物理性质测试结果表明,黏度随Al2O3质量分数增大而升高,随碱度的升高而降低;表面张力随Al2O3质量分数的增大而减小,随碱度的升高而增大,这与熔渣微观结构转变行为相符.探讨了渣金界面反应对模铸保护渣微观结构、物理性质及卷渣行为的影响.

关键词: 保护渣;模铸;微观结构;拉曼光谱;物理性质

Abstract: In order to clarify the influence mechanism of chemical composition change on physical properties of mold flux for ingot casting, the microstructure of CaO-SiO2-Al2O3-Na2O-MgO system slags were analyzed via Raman spectroscopy. The melt structure analysis results showed that there are five silicon oxygen tetrahedral structures Q0Si,Q1Si,Q2Si,Q3Si and Q4Si and three aluminum oxygen tetrahedral structures Q2Al,Q3Al and Q4Al in the slag. With the increase of basicity and the decrease of Al2O3 mass fraction, the tetrahedral structure with high degree of polymerization changes to low degree of polymerization, the number of non bridging oxygen in the slag increases and the degree of polymerization decreases. The physical property test results showed that the viscosity increases with the increase of Al2O3 mass fraction and decreases with the increase of basicity. The surface tension decreases with the increase of Al2O3 mass fraction and increases with the increase of basicity, which is consistent with the microstructure transformation behavior of slag. The effects of slag metal interfacial reaction on the microstructure, physical properties and behavior of slag entrapment are discussed.

Key words: mold flux; ingot casting; microstructure; Raman spectrum; physical property