东北大学学报:自然科学版 ›› 2020, Vol. 41 ›› Issue (10): 1394-1401.DOI: 10.12068/j.issn.1005-3026.2020.10.005

• 材料与冶金 • 上一篇    下一篇

挤压锻温度对固态再生H11钢组织和性能的影响

刘兴刚1, 王亚琴1, 马召俊2, 张德良1   

  1. (1.东北大学 材料科学与工程学院, 辽宁 沈阳110819; 2.歌尔股份有限公司, 山东 潍坊261000)
  • 收稿日期:2020-04-07 修回日期:2020-04-07 出版日期:2020-10-15 发布日期:2020-10-20
  • 通讯作者: 刘兴刚
  • 作者简介:刘兴刚(1967-),男,甘肃会宁人,东北大学副教授; 张德良(1964-),男,黑龙江兰西人,东北大学教授,博士生导师.
  • 基金资助:
    国家自然科学基金资助项目(51874080).

Effect of Extrusion-Forging Temperature on Microstructure and Mechanical Properties of Solid State Regenerated H11 Steel

LIU Xing-gang1, WANG Ya-qin1, MA Zhao-jun2, ZHANG De-liang1   

  1. 1.School of Materials Science & Engineering, Northeastern University, Shenyang 110819, China; 2. Goertek Co., Ltd., Weifang 261000, China.
  • Received:2020-04-07 Revised:2020-04-07 Online:2020-10-15 Published:2020-10-20
  • Contact: WANG Ya-qin
  • About author:-
  • Supported by:
    -

摘要: 以回收的H11钢车削屑获得的粉末为原料, 利用粉末压坯和挤压锻工艺制备样品, 并结合拉伸实验、硬度测试、XRD,SEM,TEM等分析手段, 研究了1100~1220℃不同挤压锻温度对固态再生H11钢组织结构和力学性能的影响. 结果表明:样品固结效果良好;挤压锻温度为1220℃时, 材料密度可达95.8 %;挤压锻温度达到1140℃后,基体中析出Fe7C3相; 随着挤压锻温度从1100℃升高至1220℃, 沿挤压方向的硬度从2.5GPa增加至4.4GPa, 抗拉强度从451MPa增加至808MPa, 但延伸率从3.1 %降低至0.7 %.

关键词: H11钢, 挤压锻温度, 热作模具钢, 固态再生, 车削屑

Abstract: Using the powders from the recovered machining chips of H11 steel as raw materials, the samples were prepared by powder compacting and extrusion-forging processes. Using tensile test, hardness test, XRD, SEM, TEM and etc., the effects of different extrusion-forging temperatures in a range of 1100~1220℃ on the microstructure and mechanical properties of solid regenerated H11 steel were studied. The results show that the sample has a good consolidation effect. When the extrusion-forging temperature is 1220℃, the density of the sample can reach up to 95.8%. After the temperature is over 1140℃, the Fe7C3 phase precipitates in the matrix. With increasing extrusion-forging temperature from 1100℃ to 1220℃, the hardness along the extrusion direction increases from 2.5GPa to 4.4GPa and the tensile strength increases from 451MPa to 808MPa, while the elongation decreases from 3.1% to 0.7%.

Key words: H11 steel, extrusion-forging temperature, thermal die steel, solid state regeneration, turning chips