Journal of Northeastern University(Natural Science) ›› 2024, Vol. 45 ›› Issue (3): 337-345.DOI: 10.12068/j.issn.1005-3026.2024.03.005
• Materials & Metallurgy • Previous Articles Next Articles
Lei ZHANG1,2, Kai-xi JIANG1,3, Feng XIE1, Dian-kun LU1()
Received:
2022-11-07
Online:
2024-03-15
Published:
2024-05-17
Contact:
Dian-kun LU
About author:
LU Dian-kun, E-mail: ludk@smm.neu.edu.cnCLC Number:
Lei ZHANG, Kai-xi JIANG, Feng XIE, Dian-kun LU. Reduction Behaviors of Copper, Cobalt and Iron in Smelting of Copper Oxide Concentrate[J]. Journal of Northeastern University(Natural Science), 2024, 45(3): 337-345.
温度 | Cu2O+CO(g)=2Cu+CO2(g) | CoO+CO(g)=Co+CO2(g) | FeO+CO(g)=Fe+CO2(g) | |||||||
---|---|---|---|---|---|---|---|---|---|---|
℃ | ||||||||||
1 273 | 3.99×106 | 1.00 | 1.00 | 13.27 | 0.93 | 1.08 | 0.428 | 0.30 | 3.34 | |
1 373 | 1.41×106 | 1.00 | 1.00 | 9.58 | 0.91 | 1.10 | 0.383 | 0.28 | 3.61 | |
1 473 | 5.68×105 | 1.00 | 1.00 | 7.29 | 0.88 | 1.14 | 0.348 | 0.26 | 3.87 | |
1 573 | 2.15×105 | 1.00 | 1.00 | 5.75 | 0.85 | 1.17 | 0.319 | 0.24 | 4.13 | |
1 673 | 9.16×104 | 1.00 | 1.00 | 4.66 | 0.82 | 1.21 | 0.288 | 0.22 | 4.47 | |
1 773 | 4.28×104 | 1.00 | 1.00 | 3.89 | 0.80 | 1.26 | 0.244 | 0.20 | 5.10 |
Table 2 Relationship between CO coefficient required by MO and temperatures under standard state
温度 | Cu2O+CO(g)=2Cu+CO2(g) | CoO+CO(g)=Co+CO2(g) | FeO+CO(g)=Fe+CO2(g) | |||||||
---|---|---|---|---|---|---|---|---|---|---|
℃ | ||||||||||
1 273 | 3.99×106 | 1.00 | 1.00 | 13.27 | 0.93 | 1.08 | 0.428 | 0.30 | 3.34 | |
1 373 | 1.41×106 | 1.00 | 1.00 | 9.58 | 0.91 | 1.10 | 0.383 | 0.28 | 3.61 | |
1 473 | 5.68×105 | 1.00 | 1.00 | 7.29 | 0.88 | 1.14 | 0.348 | 0.26 | 3.87 | |
1 573 | 2.15×105 | 1.00 | 1.00 | 5.75 | 0.85 | 1.17 | 0.319 | 0.24 | 4.13 | |
1 673 | 9.16×104 | 1.00 | 1.00 | 4.66 | 0.82 | 1.21 | 0.288 | 0.22 | 4.47 | |
1 773 | 4.28×104 | 1.00 | 1.00 | 3.89 | 0.80 | 1.26 | 0.244 | 0.20 | 5.10 |
Cu | Co | S | FeO | CaO | MgO | Al2O3 | SiO2 |
---|---|---|---|---|---|---|---|
20.92 | 0.23 | 0.82 | 1.94 | 2.91 | 5.99 | 4.65 | 39.08 |
Table 3 Main components of copper oxide concentrate
Cu | Co | S | FeO | CaO | MgO | Al2O3 | SiO2 |
---|---|---|---|---|---|---|---|
20.92 | 0.23 | 0.82 | 1.94 | 2.91 | 5.99 | 4.65 | 39.08 |
m(CaO)/m(SiO2) | 还原率/% | 产率/% | |||||||
---|---|---|---|---|---|---|---|---|---|
g·g-1 | Cu | Co | Fe | 金属 | 炉渣 | ||||
0.2 | 99.39 | 98.38 | 54.54 | 1.28 | 1.39 | 32.60 | 74.47 | ||
0.3 | 99.59 | 98.30 | 60.27 | 1.41 | 1.60 | 32.33 | 78.07 | ||
0.4 | 99.00 | 98.31 | 55.46 | 1.30 | 1.42 | 37.13 | 77.60 | ||
0.5 | 99.38 | 98.11 | 43.73 | 1.02 | 1.03 | 31.53 | 86.87 | ||
0.6 | 99.56 | 97.99 | 39.04 | 0.91 | 0.89 | 29.13 | 92.40 | ||
0.7 | 99.07 | 96.62 | 41.47 | 0.97 | 0.96 | 28.80 | 97.07 |
Table 4 Effect of m(CaO)/m(SiO2) on the reduction smelting index with m(FeO)/m(SiO2)= 0.71
m(CaO)/m(SiO2) | 还原率/% | 产率/% | |||||||
---|---|---|---|---|---|---|---|---|---|
g·g-1 | Cu | Co | Fe | 金属 | 炉渣 | ||||
0.2 | 99.39 | 98.38 | 54.54 | 1.28 | 1.39 | 32.60 | 74.47 | ||
0.3 | 99.59 | 98.30 | 60.27 | 1.41 | 1.60 | 32.33 | 78.07 | ||
0.4 | 99.00 | 98.31 | 55.46 | 1.30 | 1.42 | 37.13 | 77.60 | ||
0.5 | 99.38 | 98.11 | 43.73 | 1.02 | 1.03 | 31.53 | 86.87 | ||
0.6 | 99.56 | 97.99 | 39.04 | 0.91 | 0.89 | 29.13 | 92.40 | ||
0.7 | 99.07 | 96.62 | 41.47 | 0.97 | 0.96 | 28.80 | 97.07 |
m(FeO) | 入炉FeO质量/g | a | ||||
---|---|---|---|---|---|---|
m(SiO2) | ||||||
0.41 | 15.92 | 73.05 | 57.98 | 1.26 | 1.36 | 2.59 |
0.56 | 21.91 | 72.82 | 48.25 | 1.51 | 1.77 | 2.16 |
0.71 | 27.90 | 55.46 | 42.69 | 1.30 | 1.42 | 1.91 |
0.79 | 30.89 | 55.56 | 40.72 | 1.36 | 1.53 | 1.82 |
0.87 | 33.89 | 36.19 | 39.10 | 0.93 | 0.91 | 1.75 |
0.94 | 36.89 | 37.71 | 37.74 | 1.00 | 1.00 | 1.69 |
1.02 | 39.88 | 28.2 | 36.59 | 0.77 | 0.72 | 1.64 |
1.10 | 42.87 | 28.96 | 35.60 | 0.81 | 0.77 | 1.59 |
1.17 | 45.87 | 19.06 | 34.73 | 0.55 | 0.49 | 1.55 |
1.25 | 48.87 | 15.05 | 33.97 | 0.44 | 0.38 | 1.52 |
Table 5 Effect of m(FeO)/m(SiO2) on the reduction smelting index with m(CaO)/m(SiO2)=0.4
m(FeO) | 入炉FeO质量/g | a | ||||
---|---|---|---|---|---|---|
m(SiO2) | ||||||
0.41 | 15.92 | 73.05 | 57.98 | 1.26 | 1.36 | 2.59 |
0.56 | 21.91 | 72.82 | 48.25 | 1.51 | 1.77 | 2.16 |
0.71 | 27.90 | 55.46 | 42.69 | 1.30 | 1.42 | 1.91 |
0.79 | 30.89 | 55.56 | 40.72 | 1.36 | 1.53 | 1.82 |
0.87 | 33.89 | 36.19 | 39.10 | 0.93 | 0.91 | 1.75 |
0.94 | 36.89 | 37.71 | 37.74 | 1.00 | 1.00 | 1.69 |
1.02 | 39.88 | 28.2 | 36.59 | 0.77 | 0.72 | 1.64 |
1.10 | 42.87 | 28.96 | 35.60 | 0.81 | 0.77 | 1.59 |
1.17 | 45.87 | 19.06 | 34.73 | 0.55 | 0.49 | 1.55 |
1.25 | 48.87 | 15.05 | 33.97 | 0.44 | 0.38 | 1.52 |
焦比/% | 质量分数/% | n(O)/n(Si) | |||||
---|---|---|---|---|---|---|---|
CaO | MgO | Al2O3 | FeO | SiO2 | |||
2 | 14.47 | 5.59 | 10.20 | 24.38 | 37.88 | 0.410 | 3.76 |
4 | 17.71 | 6.85 | 9.18 | 25.19 | 43.34 | 0.436 | 3.55 |
5 | 20.43 | 8.26 | 9.15 | 11.33 | 48.64 | 0.497 | 3.23 |
6 | 18.09 | 6.92 | 11.30 | 21.87 | 45.72 | 0.455 | 3.49 |
8 | 19.84 | 7.94 | 9.86 | 16.21 | 52.2 | 0.498 | 3.23 |
10 | 20.90 | 8.34 | 9.20 | 11.94 | 51.55 | 0.506 | 3.19 |
Table 6 Slag composition with m(FeO)/m(SiO2)=0.71 and m(CaO)/m(SiO2)=0.4 under various coke rates
焦比/% | 质量分数/% | n(O)/n(Si) | |||||
---|---|---|---|---|---|---|---|
CaO | MgO | Al2O3 | FeO | SiO2 | |||
2 | 14.47 | 5.59 | 10.20 | 24.38 | 37.88 | 0.410 | 3.76 |
4 | 17.71 | 6.85 | 9.18 | 25.19 | 43.34 | 0.436 | 3.55 |
5 | 20.43 | 8.26 | 9.15 | 11.33 | 48.64 | 0.497 | 3.23 |
6 | 18.09 | 6.92 | 11.30 | 21.87 | 45.72 | 0.455 | 3.49 |
8 | 19.84 | 7.94 | 9.86 | 16.21 | 52.2 | 0.498 | 3.23 |
10 | 20.90 | 8.34 | 9.20 | 11.94 | 51.55 | 0.506 | 3.19 |
焦比/% | 焦炭利用率占比/% | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Cu | Fe | ||||||||||
2 | 12.98 | 18.79 | 0.84 | 0.69 | 0.63 | 66.41 | 18.23 | ||||
4 | 22.55 | 34.71 | 1.55 | 0.65 | 0.59 | 56.98 | 15.83 | ||||
5 | 55.46 | 42.67 | 1.91 | 1.30 | 1.42 | 47.12 | 31.14 | ||||
6 | 32.13 | 50.63 | 2.26 | 0.63 | 0.57 | 39.19 | 15.03 | ||||
8 | 53.68 | 66.56 | 2.98 | 0.81 | 0.76 | 29.53 | 18.84 | ||||
10 | 64.83 | 82.48 | 3.69 | 0.79 | 0.74 | 23.34 | 18.20 |
Table 7 Effect of coke rate on iron reduction and coke utilization with m(FeO)/m(SiO2)=0.71 and m(CaO)/m(SiO2)=0.4
焦比/% | 焦炭利用率占比/% | ||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Cu | Fe | ||||||||||
2 | 12.98 | 18.79 | 0.84 | 0.69 | 0.63 | 66.41 | 18.23 | ||||
4 | 22.55 | 34.71 | 1.55 | 0.65 | 0.59 | 56.98 | 15.83 | ||||
5 | 55.46 | 42.67 | 1.91 | 1.30 | 1.42 | 47.12 | 31.14 | ||||
6 | 32.13 | 50.63 | 2.26 | 0.63 | 0.57 | 39.19 | 15.03 | ||||
8 | 53.68 | 66.56 | 2.98 | 0.81 | 0.76 | 29.53 | 18.84 | ||||
10 | 64.83 | 82.48 | 3.69 | 0.79 | 0.74 | 23.34 | 18.20 |
元素 | 谱图1 | 谱图2 | 谱图3 | |||
---|---|---|---|---|---|---|
质量 分数 | 原子 分数 | 质量 分数 | 原子 分数 | 质量 分数 | 原子 分数 | |
O | 43.54 | 59.96 | 32.06 | 57.14 | — | — |
Mg | 7.15 | 6.48 | 0.88 | 1.03 | — | — |
Al | 6.27 | 5.12 | — | — | — | — |
Si | 21.63 | 16.97 | 14.07 | 14.29 | — | — |
Ca | 19.33 | 10.63 | 2.36 | 1.68 | — | — |
Fe | 1.80 | 0.71 | 50.63 | 25.86 | 85.84 | 87.34 |
Ti | 0.28 | 0.13 | — | — | — | — |
Cu | — | — | — | — | 14.16 | 12.66 |
Table 8 Element analysis of EDS spectrum points in Fig.8
元素 | 谱图1 | 谱图2 | 谱图3 | |||
---|---|---|---|---|---|---|
质量 分数 | 原子 分数 | 质量 分数 | 原子 分数 | 质量 分数 | 原子 分数 | |
O | 43.54 | 59.96 | 32.06 | 57.14 | — | — |
Mg | 7.15 | 6.48 | 0.88 | 1.03 | — | — |
Al | 6.27 | 5.12 | — | — | — | — |
Si | 21.63 | 16.97 | 14.07 | 14.29 | — | — |
Ca | 19.33 | 10.63 | 2.36 | 1.68 | — | — |
Fe | 1.80 | 0.71 | 50.63 | 25.86 | 85.84 | 87.34 |
Ti | 0.28 | 0.13 | — | — | — | — |
Cu | — | — | — | — | 14.16 | 12.66 |
1 | Fay I, Barton M D.Alteration and ore distribution in the Proterozoic mines series,Tenke‐Fungurume Cu‐Co district,Democratic Republic of Congo[J].Mineralium Deposita,2012,47(5):501-519. |
2 | 周灼刚.用密闭鼓风炉熔炼氧化铜矿方法浅析[J].世界有色金属,2000(9):9-13. |
Zhou Zhuo‐gang.Analysis on the method of smelting copper oxide in a closed blast furnace[J].World Nonferrous Metals,2000(9):9-13. | |
3 | Hauptmann A.The archaeometallurgy of copper [M].Berlin:Springer,2007:217-254. |
4 | 苏凤来.降低密闭鼓风炉还原熔炼氧化铜矿炉渣品位的探讨[J].有色金属(冶炼部分),2017,39(9):12-14. |
Su Feng‐lai.Discussion on reducing grade of copper smelting slag by reduction smelting in closed blast furnace[J].Nonferrous Metals (Extractive Metallurgy),2017,39(9):12-14. | |
5 | 陈静,石晓波,龚丽维,等.碱式碳酸铜的制备[J].大学化学,2012,27(5):78-82. |
Chen Jing, Shi Xiao‐bo, Gong Li‐wei,et al.Preparation of basic copper carbonate[J].University Chemistry,2012,27(5):78-82. | |
6 | Li Y, Ren J, Wei H,et al.Reduction kinetics of cold‐bonded briquette prepared from return fines of sinter with carbon monoxide and coke[J].Steel Research International,2023,94(8):1-14. |
7 | Turkdogan E T, Vinters J V.Effect of carbon monoxide on the rate of oxidation of charcoal,graphite and coke in carbon dioxide[J].Carbon,1970,8(1):39-53. |
8 | Alain V.Extractive metallurgy 2—metallurgical reaction processes[M].London:ISTE Ltd,2011. |
9 | Alain V.Extractive metallurgy 1—basic thermodynamics and kinetics [M].London:ISTE Ltd,2011. |
10 | ASM International Alloy Phase Diagram and the Handbook Committees.ASM handbook:alloy phase diagrams[M]. Portland:ASM International,1992. |
11 | Xiao W B, Yao S W, Zhou S W,et al.Evolution of the structure and viscosity of copper slag during metallization‐reduction[J].Journal of Alloys and Compounds,2022,903:163751. |
12 | Li B W, He M S, Huang J Y .Characteristics of anorthite‐pyroxene ceramics made from hot‐poured steelmaking slag[J].JOM,2017,69(2):173-177. |
13 | Wu G X, Yazhenskikh E, Hack K,et al.Viscosity model for oxide melts relevant to fuel slags.part 2:the system SiO2-Al2O3-CaO-MgO-Na2O-K2O[J].Fuel Processing Technology,2015,138:520–533. |
14 | Hack K, Wu G X, Yazhenskikh E,et al.A CALPHAD approach to modelling of slag viscosities[J].Computer Coupling of Phase Diagrams and Thermochemistry,2019,65:101-110. |
15 | 王震,姜茂发,刘承军,等.CaO-SiO2-Al2O3-Na2O-MgO系模铸保护渣微观结构解析[J].东北大学学报(自然科学版),2023,44(4):517-523. |
Wang Zhen, Jiang Mao‐fa, Liu Cheng‐jun,et al.Microstructure analysis of mold flux of CaO‐SiO2‐Al2O3‐Na2O‑MgO system for ingot casting[J].Journal of Northeastern University(Natural Science),2023,44(4):517-523. |
[1] | Yu-ting FENG, Li CHENG, Ke-mei WANG, En-zhu HU. Effect of Metallic Minerals on Transport Characteristics of Ammonium Dibutyl Dithiophosphate in Saturated Porous Media [J]. Journal of Northeastern University(Natural Science), 2024, 45(3): 401-406. |
[2] | GUO Jin-ming, YANG Hong-ying, TONG Lin-lin, MENG Jing. Study on Process Mineralogy of a Copper-Molybdenum Mixed Concentrate in Tibet [J]. Journal of Northeastern University(Natural Science), 2023, 44(8): 1195-1200. |
[3] | WEI Zuo-an, XIE Jin-xin, ZHAO Jun-kang, LU Ting. Effect of Chemical Dust Suppressants on Suitability of Herbaceous Plants in Copper Tailings Ponds [J]. Journal of Northeastern University(Natural Science), 2022, 43(12): 1799-1804. |
[4] | ZHAO Bing, ZHANG Ran, XU Xin-yang. Magnetic Bio-char Derived from Sewage Sludge and Its Adsorption Ability for Cu(Ⅱ) in Aqueous System [J]. Journal of Northeastern University(Natural Science), 2021, 42(7): 1012-1018. |
[5] | XIAO Fa-xin, PENG Yu, SUN Shu-chen, TU Gan-feng. Leaching of High-Alkaline Gangue Low-Grade Copper Oxide Ore in (NH4)2SO4-NH3-H2O Solution [J]. Journal of Northeastern University(Natural Science), 2021, 42(6): 795-801. |
[6] | ZHANG Pei-hong, YUAN Wei, WEI Zhong-yuan, LI Zi-jian. Thermal Runaway Analysis of NCM Lithium-Ion Battery in Humid and Hot Environment [J]. Journal of Northeastern University Natural Science, 2020, 41(6): 881-887. |
[7] | CHEN Jing-qi, LIU Xiang-hua, YAN Shu, YU Qing-bo. Experimental Study on Bending Capacity of Copper/Steel/Copper Cold Rolled Composite Strip [J]. Journal of Northeastern University Natural Science, 2019, 40(5): 647-652. |
[8] | MA Xiao-gang, CHEN Liang-yu, LI Yang. Optimization of Longevity Technology for Bosh Copper Cooling Stave with Shaped Tubes Based on Response Surface Method [J]. Journal of Northeastern University Natural Science, 2019, 40(5): 710-715. |
[9] | WANG Gai-rong, YANG Hong-ying, TONG Lin-lin, LIU Yuan-yuan. Research on Technological Mineralogy of Copper Oxide Ore in Luanshya, Zambia [J]. Journal of Northeastern University Natural Science, 2019, 40(3): 350-355. |
[10] | JIANG Liang-you, WEI De-zhou, LIU Kai-kai, ZHANG Hao. Kinetics of Bioleaching for Copper Sulfide Ore with Different Grade [J]. Journal of Northeastern University Natural Science, 2019, 40(10): 1491-1495. |
[11] | QIU Xue-min, YANG Hong-ying, CHEN Guo-bao, ZHAO Su-xing. Interface Characteristics of Lead and Copper Minerals from Ultra-fine Cyanide Tailings [J]. Journal of Northeastern University Natural Science, 2019, 40(1): 58-62. |
[12] | LI Xiao-long, LIU Yan, WANG Dong-xing, ZHANG Ting-an. Physical Simulation of Emulsion Phenomena in Copper Side-blown Smelting Process [J]. Journal of Northeastern University Natural Science, 2018, 39(5): 649-653. |
[13] | WANG Jian, LIU Zi-long, CHEN Guo-bao, YANG Hong-ying. Consumption Mechanism of Sodium Sulfide in Flotation Separation of Copper and Molybdenum [J]. Journal of Northeastern University Natural Science, 2018, 39(3): 362-366. |
[14] | LIU Yuan-yuan, YANG Hong-ying, TONG Lin-lin, JIN Zhe-nan. Novel Hydrometallurgical Process of Refractory Copper-Cobalt Ores from Zambia [J]. Journal of Northeastern University Natural Science, 2017, 38(9): 1285-1288. |
[15] | YU Lin-xin, WANG Da-zhi, LI Shuo, ZHENG Di. Loss Calculation and Analysis of Efficient Permanent Magnet Coupler [J]. Journal of Northeastern University Natural Science, 2017, 38(11): 1524-1529. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||